(1) Wrong Yarn

Appearance: In the hair of the knitted fabric, laterally continuous terry loops are woven from coarser or finer yarns of a larger gauge. Most of them are single roots, but even there are parallels or multiple roots. According to the dense, thick and normal are different.

Cause: When weaving knitted fabrics, operators mistakenly use non-specified counts or yarns of Danny size for knitting. Misuse of the finer yarns makes the fabric appear thinner. Misuse of thicker yarns results in thicker fabrics.

(2) Wrong End

Appearance: The warp yarns of woven fabrics have a single or side-by-side thickness that is not specified. If it is a fine yarn, it is called Fine End. If it is a thicker yarn, it is called Coarse End.

Contributing factors: The number of bobbin yarns involved in the warping of the menstruation was incorrect and the warp yarns were not specified. This kind of embarrassment is often full-pepper.

(3) Wrong Pick

Appearance: The weft of the woven fabric has one or more thicknesses that are not specified. For finer yarns, FinePick is called. If it is a thicker yarn, it is called Coarse Pick.

Causes: When weaving, the weft yarn of the weft tube, or the number of bobbin yarns fed by the shuttleless weaving machine is wrong, and we use the weft yarn that is not specified. After the operator discovered it, it was removed and shut down. However, weaving machines that change tubes automatically are often not easy to find.

(4) Wrong Weaving

Appearance: The weave method is wrong, and the texture of the cloth is different from that of the original designer. For example, the left twill is woven into a right twill.

Causes: Mostly caused by wearing errors. Others, such as jacquard fabrics are incorrect, warp yarns are misaligned in multi-standard warp fabrics.

(5) Wrong Draw

Appearance: Two warp yarns that are adjacent to each other are woven together into one fabric. Regardless, the root (actually two) yarns appear particularly thick. Such crickets are all perfectly matched. If they are found in the primary weaving of the warp beam, removing one of the roots in the tandem can be completely avoided.

Causes: 1) When neglecting the warp draft, it is negligence to treat two strands as one. 2) After the sizing, the yarn is not clear, the two stick together and form the same root. 3). Two threads penetrate the same heddle at the time of threading.

(6) Mispick

Appearance: Two wefts are woven into the same weaving mouth and even have three or more roots. The length of the parallel weft ranges from the full width of the fabric to more than 10 centimeters near the edge of the cloth.

Causes: 1). The length of the fabric is full and weft. After troubleshooting due to shutdown, we did not check the weaving drive. Or the weft pin failed and the weft break did not stop. 2). Non-full-width latitude and longitude, due to the length of the insurance yarn is not enough, the side cut is not set properly or sharp enough, and the end of the yarn is not removed after weft break.

(7) Pick-Out Mark

Appearance: The weft of the weft cloth is not well dismantled. After weaving continues, there are still marks on the cloth surface.

Causes: In the weaving of fabrics, the operators found that wefts were weaving at different places, or weaving severe roads and thinning. We immediately shut down the wefts that weaved in and cut them out. When the warp yarn is removed, the warp yarn is rubbed off by the weft yarn, resulting in a large amount of hairiness. Therefore, after reweaving, the warp yarn exhibits a width-equivalent multi-hairiness cloth surface in the scope of original dismantling.

(8) Broken End

Appearance: The warp of the fabric breaks one or more roots, resulting in a large distance between the two adjacent yarns. In plain weave fabric, it becomes two broken yarns juxtaposed, as if by. In twill weaves, there is a phenomenon of discontinuity.

Causes: The warp yarn is interrupted by weaving and the stopping device fails. Weaving continues without weaving the warp yarn.

(9) Broken Pick

Appearance: The weft yarn in the fabric breaks, but the distance between the ends of the break is very short, ie the length of the cut off is small. This type of defect is generally not significant.

Causes: 1) The weft yarn breaks in the weaving but it continues to weave in a moment, only a short distance away. 2). There are serious rough knots and flying flowers on the weft yarn, which causes the weft to break when it is removed.

(10) 100 feet (lacking)

Appearance: This kind of flaw only occurs in the twill weave, in the warp of the same part of each complete organization, at the same time floating on the surface of the cloth, it resembles a set of many feet.

Causes: When a twill weaves less weft yarn, the interweaving point decreases, and part of the warp yarn floats on the weft yarn twice.

(11) End Snarl

Appearance: One of the warp yarns in the fabric has a small amount of curling and twisting and weaving into the cloth. Fabrics made from strong twisted yarns are more likely to occur.

Causes: One of the root warp yarns was loose during warping, causing a period of curling.

(12) Filling Snarl

Appearance: Fabric weft yarns have a small amount of curling and weaving into the fabric. Fabrics made from strong twisted yarns are more likely to occur.

Causes: 1) In the weft bobbin or in the bobbin yarn used for the weft yarn, the small yarn is already curled up. 2). The weft bobbin is improperly formed and it is not smooth when the yarn is unreeled. 3). The tension of the weft yarn is too small, and the mouth of the weaving is not clear.

(13) Reed Mark

Appearance: Between the two warp yarns, there is a large gap between the two warp yarns, and weaving weft yarns can be seen.

Causes: 1) The deformation of the steel rakes has failed to control the warp yarns in position, or the dents have loosened. 2). There are one or a few gaps in the warp yarn and the tension applied during weaving is too large.

(14) Temple Mark

Appearance: Approximately 2 to 5 cm wide acupuncture or traces of acupuncture in the cloth. In severe cases, the weft yarns of the part are wavy and curved.

Cause: The thickness of the needle used in the temple supporter is not appropriate, and the stall supporter stuck in the ring cannot be rotated, or the rotation is not smooth enough.

(15) Connector (Knot)

Appearance: Thick and round ball with tight knotting on the fabric.

Cause: After the warp or weft breaks and joins, the knots hit are too large to protrude from the fabric.

(16) Float

Appearance: warp or weft yarns are not woven in accordance with the specified organization, but float on the surface.

Cause: The angle at which the weaving mouth is opened is too small, or the heald wire is suspended unevenly, and a few warp yarns are particularly loose.

(17) Weaving Hole

Appearance: The warp and weft yarns of the embroidered fabric break, forming holes of different sizes. This kind of flaws can easily occur in fabrics with relatively longitude and latitude.

Causes: The friction of the shuttle, the licker-in holding the fishing hook, will cause the warp and weft to break. In addition, the warp can also break the warp.

(18) Slack End

Appearance: The warp yarn weaves into the cloth, in the interweaving point, is convex and concave on the surface of the cloth, and it is arched upward. Generally speaking, it is called ribs in the factory.

Causes: The warp yarns of a single warp are under less tension during weaving, or the warp yarns are too loose after the warp yarns are joined.

(19) Slack Filing

Appearance: A weft yarn that is woven into a cloth, at the point of its intertwining, protrudes from the cloth more than normal and has a phenomenon of upward arching. Generally not obvious.

Cause: A single weft yarn has less tension when weaving.


For more content, please follow this site

180 Design Synthetic Leather

180 Design Synthetic Leather,Synthetic Leather With Dot Design,Latest Design Soft Synthetic Leather,180 Angle Synthetic Leather

Shaoxing Dongtai Polymeric Materials Co.,Ltd , https://www.sxdtmaterials.com